Porosity caused due to entrapment of air in the mold is?
- Suck back porosity
- Back pressure porosity (Correct Answer)
- Localized shrinkage porosity
- Pin hole porosity
Explanation
Classification of porosity in casting alloy:
- Caused due to solidification shrinkage of alloy:
a.Localized shrinkage porosity or shrink-spot porosity:
Premature termination of flow of molten metal during solidification when sprue freezes before rest of casting.
Large irregular voids at junction of sprue former of the casting.
Avoid by using sprue of correct thickness, use of
reservoir, attach the sprue to thickest portion of wax pattern & avoid excess length ofsprue.
During cooling sequence, sprue should freeze last,
b.Suck back porosity:
Variation of localized shrinkage porosity due to molten
metal impinging from sprue channel on mold wall
creating a hot spot (region of high molten temp.) External void inside of a crown opposite the sprue. Avoided by giving flare at sprue attachment and reducing temperature difference between mold & molten alloy.
c.lificroporosity: due to rapid solidification.
Caused due to trapped gas in the casting during
shrinkage
a, Gas inclusion porosity: spherical in shape or larger than pin hole porosity. Avoid by melting (alloy gold) in
reducing zone o flame.
b. Pin hole porosity: spherical porosities smaller than
gas inclusion. Avoid by prernelting gold alloy in graphite crucible.